Monel Chemical Properties

Grades Ni% C% Ti% Ai% Cu% Fe% Sonstige Autres-Other %
Alloy 400 65.0 0.12 - - 32.0 1.5 Mn 1.0
Alloy K 500 64.0 0.13 0.6 2.8 30.0 1.0 Mn 0.8
Alloy R 405 66.0 0.15 - - 31.0 1.2 Mn 1.0; S 0.04


Monel k500

Typical Room Temperature Tensile Properties of Annealed Material

Product Form Condition Tensile (ksi) .2% Yield (ksi) Elongation % Hardness
Rod & Bar Hot-Finished / Aged 140-190 100-150 30-20 27-38 HRC
Rod & Bar Hot Finished / Annealed 90-110 40-60 45-25 75-90 HRB
Rod & Bar Hot Finished / Annealed / Aged 130-165 85-120 35-20 24-35 HRC
Rod & Bar Cold-Drawn / Aged 135-185 95-160 30-15 25-41 HRC
Rod & Bar Cold-Drawn / Annealed / Aged 130-190 85-120 30-20 24-35 HRC
Plate Hot-Finished / Aged 140-180 100-135 30-20 27-37 HRC
Sheet Cold-Rolled / Annealed 90-105 40-65 45-25 85 HRB Max


Monel 400

Typical Room Temperature Tensile Properties of Annealed Material

Product Form Condition Tensile (ksi) .2% Yield (ksi) Elongation (%) Hardness (HRB)
Rod & Bar Annealed 75-90 25-50 60-35 60-80
Rod & Bar Cold-Drawn Stress Relieved 84-120 55-100 40-22 85-20 HRC
Plate Annealed 70-85 28-50 50-35 60-76
Sheet Annealed 70-85 30-45 45-35 65-80
Tube & Pipe Seamless Annealed 70-85 25-45 50-35 75 max*